A rotor that measures well on total flux can still be a bad rotor. The number that predicts whether a motor will whine at 4,000 rpm is not the average field — it is the distribution: how much poles differ from each other, and how much the waveform departs from a sine.
Measuring that distribution is a different engineering problem from measuring a field strength, and the two available routes — a single scanning probe and a multi-channel Hall array — trade resolution against throughput in a way that is often decided by procurement rather than by the measurement requirement.
What is the difference between single-probe scanning and Hall array mapping?
A hall probe multi axis scanner moves one calibrated three-axis sensor over the rotor on an encoded stage: highest positional accuracy and a fully traceable worst-case number, at minutes per rotor. A Hall sensor array captures an entire pole or circumference at once: seconds per rotor and viable 100 % inspection, but spatial resolution is fixed by channel pitch and channels must be calibrated against each other.
Key takeaways
- Field strength is a single number; the failure modes are all distributions. Pole-to-pole asymmetry, waveform harmonics, skew and local defects cannot be seen in an average, and an average is what a simple gauss meter gives you.
- Positioning dominates the uncertainty, not sensor accuracy. Near-field harmonics decay exponentially with distance from the surface, so a small gap error changes the reading far more than the sensor’s own linearity does.
- The two methods answer different questions. Scanning is the reference method for qualification and dispute resolution; arrays are the production method for 100 % screening. Choosing one and calling it “the” method is how a plant ends up screening for the wrong defect.
- Pole asymmetry and flux THD map onto specific vehicle symptoms — unbalanced magnetic pull drives pole-pass vibration, harmonic content drives torque ripple and cogging, and back-EMF imbalance drives circulating currents in parallel paths.
- A measurement report without an uncertainty statement and a stated sensor-to-surface distance is not evidence. It is a number with no error bar, and it will not survive a supplier dispute.
1. Multi-axis magnetic flux density testing: what is actually being measured
1.1 Two components, two different stories
A surface field map is usually described as “the field at the rotor surface”. In practice, a three-axis sensor records three orthogonal components, and two of them carry most of the diagnostic information:
- Normal component (radial, in rotor coordinates) — the flux that crosses the air gap and produces torque. This is the component that predicts back-EMF and torque constant.
- Tangential component — the component associated with the field’s spatial phase. It reveals skew errors and magnetization-direction errors that leave the normal component’s amplitude almost intact.
A single-axis gauss meter measures one component at one position. That is sufficient for a coarse go/no-go check on a magnet, and insufficient for anything that predicts NVH. The distinction matters commercially: a supplier quoting “surface field measured with a gauss meter” has measured a number, not a distribution.
1.2 The measurement distance problem
The field above a magnetized surface decays with distance, and it decays faster for higher spatial harmonics. A harmonic of order h with wavelength λ/h falls off as e^(−2πhz/λ). The consequence is uncomfortable:
- A small error in sensor-to-surface distance barely changes the fundamental.
- The same error changes the high harmonics substantially — and the high harmonics are exactly what diagnose local defects such as a chipped magnet corner.
So two labs measuring “the surface field” at nominally the same location can disagree by a few percent on the fundamental and by tens of percent on the harmonics. The disagreement is not a calibration failure; it is a distance failure. Any credible report states the sensor-to-surface distance and the method used to establish it.
1.3 The coordinate frame has to be declared
A rotor map is only interpretable if the frame is defined: rotor axis, pole index 1 position, angular zero reference, and the sign convention for each component. Two reports of the same rotor in different frames look like two different rotors.
For multi-pole traction rotors this is not pedantry. Pole 1 identification and the direction of rotation determine whether a “weak sector at 45°” is a manufacturing defect or a coordinate artefact, and getting it wrong sends a production team chasing a problem in the wrong station.
2. Magnetic flux inspection equipment: three routes compared
| Criterion | Single-probe scanning | Hall sensor array | Magneto-optical imaging |
|---|---|---|---|
| Principle | One 3-axis Hall sensor on an encoded stage, point by point | Multiple Hall sensors on an arc or ring, sampled simultaneously | Magneto-optical film; field imaged via polarization rotation |
| Spatial resolution | Highest — set by stage resolution and probe tip | Set by channel pitch (millimetres) | Very high, limited by optical resolution |
| Time per rotor | Minutes | Seconds | Seconds to minutes depending on field of view |
| Coverage | Full surface, arbitrary paths, multiple planes | Fixed geometry per rotor family | Limited to visible/flat or gently curved surfaces |
| Calibration burden | One sensor, one traceable chain | Every channel must be matched; drift between channels | Optical + magnetic calibration, less standardised |
| Quantitative accuracy | Highest, with full uncertainty budget | Good, dominated by channel matching and standoff | Moderate; best used for defect detection than absolute values |
| 100 % production inspection | Not viable | Yes | Seldom |
| Best suited to | Qualification, audit samples, dispute resolution, R&D | End-of-line screening, batch trend monitoring | Local defect imaging, failure analysis |
Send a rotor drawing for a measurement method recommendation →
The comparison is not a ranking. It is a division of labour, and the division follows a simple rule: use the method whose resolution matches the size of the defect you are trying to catch.
- A weak pole from a fixture asymmetry spans tens of millimetres — an array catches it easily.
- A hairline crack in one magnet’s corner spans a fraction of a millimetre — only a scanning probe or high-resolution imaging will see it, and only if the scan path crosses it.
2.1 What a hall probe multi axis scanner delivers that an array cannot
Three things, and each has a commercial consequence:

1. A defensible worst-case number. Because a single sensor traverses every point, the peak demagnetizing field and the peak flux are measured by the same device with one calibration chain. In a supplier dispute, that is the difference between an argument and a measurement. 2. Arbitrary measurement planes. Scanning can map at several axial positions, which is the only practical way to detect skew and axial non-uniformity in a skewed rotor. 3. No channel-matching error. With one sensor, there is no cross-channel gain mismatch to characterise, which removes an entire error source that array users must budget for.
The cost is throughput: minutes per rotor makes scanning a sampling tool, not a screening tool.
2.2 What a hall sensor array delivers that scanning cannot
Throughput, and the statistical power that comes with it.
An array measuring every rotor in a shift produces a distribution rather than a sample. That changes what quality control can do: trends become visible before failures appear, and the acceptance limit can be set from a population rather than from a handful of audit parts. For traction rotors built at volume, this is usually worth more than the resolution loss — provided the array is used for the defects it can actually resolve.
The array’s weakness is equally structural. Channel pitch is fixed, so a defect smaller than the pitch may be missed entirely or appear as a small amplitude reduction with no signature. An array that “passes” a rotor with a chipped magnet corner is not malfunctioning; it is being asked a question outside its resolution.
3. Rotor surface magnetic field mapping: the four metrics that predict failure
A map is data. These four derived metrics are what turn it into a decision, and each maps onto a specific vehicle-level symptom.
3.1 Pole flux asymmetry testing
The metric is the peak-to-peak spread of per-pole flux, normalised to the rotor mean:
A = (Φ_max − Φ_min) / Φ_mean × 100 %
What it predicts:
- Unbalanced magnetic pull. Poles carrying more flux pull harder, which produces a rotating radial force at the pole-pass frequency. It shows up as vibration and as bearing load, and it is audible as a tone that tracks speed.
- Circulating currents. Where a winding has parallel paths, unequal pole flux produces unequal back-EMF, and the difference drives a circulating current that heats the winding unevenly. This is often diagnosed as a winding problem before anyone measures the rotor.
A design that specifies “< 3 % asymmetry” without saying whether that is peak-to-peak over the mean, or standard deviation, has not specified anything. Both definitions appear in industry documents and they differ by a factor of two or more on the same rotor.
3.2 Flux waveform THD
The harmonic distortion of the flux waveform is computed from the spatial harmonic amplitudes:

THD = √(Σ V_h²) / V_1, for h ≥ 2
What it predicts:
- Torque ripple, because each flux harmonic interacts with the current to produce a torque component at a distinct order.
- Cogging torque at low speed, which is a comfort and position-control problem rather than an efficiency one.
- Acoustic tonal content, since stator iron responds to the same orders.
THD is the metric where the two measurement methods diverge most in practice. An array with channel pitch of a few millimetres cannot resolve harmonics whose half-wavelength approaches that pitch, so it reports a THD that omits the high orders — and those are precisely the orders associated with fine defects and with the highest acoustic frequencies.
3.3 Skew and axial phase
Skew is designed into many traction rotors to reduce cogging. It is also easily built wrong, and the error is invisible to a single-plane map: a skewed rotor measured at one axial position looks perfect.
Detecting it requires mapping at two or more axial planes and comparing the angular phase of the fundamental. A phase difference between planes that does not match the design skew indicates a build error — step-skew assembled with the wrong segments, or continuous skew applied at the wrong angle.
This is the one metric that a single-probe scanner delivers far more cheaply than an array, because the array’s fixed geometry usually constrains it to one plane.
4. Fault signature matrix
The value of a mapping programme is not the map — it is the ability to read a signature and name the cause. The matrix below is the diagnostic core of a flux mapping service.
| Signature on the map | Physical cause | Method that resolves it | Common false positive |
|---|---|---|---|
| All poles low, symmetric | Uniform under-saturation, or charging at elevated temperature | Either method | Sensor standoff too large — check distance first |
| One weak sector, same angular position on every rotor | Fixture field not reaching that region | Array (fast) or scan | Pole-indexing error between rotors |
| Alternating strong/weak poles | Pole-piece asymmetry or a defect in one magnetizing circuit leg | Array | Rotor mounted off-centre, producing a once-per-rev modulation |
| Sharp step within a single magnet | Crack or chipped corner; the gap is an air path | Scanning probe or imaging | Debris on the surface during measurement |
| Elevated specific harmonic, low asymmetry | Magnetization direction error — segmented or Halbach arrays | Scanning with harmonic analysis | Winding or test-fixture artefact in the back-EMF measurement |
| Phase shift between axial planes | Skew built at the wrong angle, or step-skew mis-assembled | Multi-plane scanning | Tilted rotor axis during measurement |
| Localised loss concentrated in one angular zone, developing over time | Thermal demagnetization in a hot region | Scanning, compared against a baseline map | Coating damage mimicking a field loss |
Ask for a sample flux map report →
Two entries in that table are worth emphasising because they account for a large share of misdiagnosis:
Alternating strong/weak poles is the classic “the fixture is bad” conclusion, and it is wrong more often than right. A rotor mounted with a small eccentricity produces a once-per-revolution modulation that looks like alternating poles when sampled at pole frequency. Re-measure with the rotor indicated true before condemning the fixture.
Elevated harmonic with normal asymmetry is the signature most often missed, because the metric that would reveal it — harmonic spectrum — is the one most often omitted from a report. A report containing only peak field and average flux cannot see this defect at all.
5. The measurement report: what makes it evidence
A flux map becomes evidence only when it carries the information needed to reproduce it. Reports that omit the following are not comparable between suppliers, batches or years.
5.1 Mandatory content
| Item | Why it is mandatory |
|---|---|
| Measurement uncertainty, expanded, with coverage factor | Without it, a 2 % difference between two rotors may be noise |
| Sensor calibration status and traceability chain | Establishes that the instrument’s reading is anchored to a standard |
| Sensor-to-surface distance and how it was established | Dominates the uncertainty on high harmonics |
| Measurement temperature | Magnetization and sensor gain both vary with temperature |
| Sampling grid or channel pitch | Defines the smallest defect the map can show |
| Coordinate frame definition and pole-1 identification | Makes the map interpretable and comparable |
| Pass/fail limits with their definition | Distinguishes peak-to-peak from standard deviation, and states the basis |
| Raw data, not only summary plots | Allows re-analysis and dispute resolution |
Request the report template and uncertainty statement →
5.2 Calibration and accreditation — state what is true
Two separate things are often conflated in marketing material:
- Calibration traceability means the instrument’s readings can be traced to a national standard through an unbroken chain. Every competent lab has this.
- Accreditation to ISO/IEC 17025 means the laboratory’s competence and quality system have been independently assessed for specific test methods.
These are not the same claim, and a report should state only what the laboratory actually holds. A supplier that implies accreditation it does not have is making a claim a customer’s quality auditor will test, and the consequence is disproportionate: an unaccredited report is still useful engineering data, but a misrepresented one destroys the credibility of everything else in the audit.
5.3 Traceability for a production programme
For a traction motor programme, the mapping data is part of the quality record and follows the rotor. Minimum requirements:
- Every map tied to a rotor serial number and a timestamp, not to a batch
- Retention for the programme’s service life plus the contractual record period, which for automotive programmes commonly means a decade or more
- Version-controlled analysis software, so a map analysed in year five can be re-analysed with the same algorithm
- A baseline map per rotor design, against which field returns can be compared
The last item is the one most often missing, and the one that matters most in a failure investigation: without a baseline from a known-good rotor of the same design, a service map cannot distinguish a manufacturing defect from a design characteristic.
6. Rotor flux sweep test: screening versus audit sampling
The practical resolution to the scanning-versus-array trade is not to choose, but to run both at different frequencies.
A typical programme structure:
- 100 % screening by array at end of line, against limits derived from the rotor’s own population, screening for the defects an array can resolve: weak poles, gross asymmetry, fixture drift, missing or mis-oriented magnets.
- Audit sampling by scanning probe, at a defined frequency per shift or per batch, including multi-plane scans for skew and harmonic analysis for waveform quality.
- Reference mapping on first article and on any process change — new fixture, new magnet lot, new bonding process — establishing the baseline that everything else is compared against.
The ratio between the two frequencies is a risk decision, and it should be justified by defect severity and detection capability rather than by cost alone. A defect that an array cannot see and that leads to a field failure justifies a higher scanning frequency than its historical occurrence rate would suggest.
7. Specifying a magnetic flux density measurement service
| Item | What to state | Why it decides the answer |
|---|---|---|
| Rotor geometry | Outer diameter, stack length, bore, mass | Sets stage travel, fixturing and handling |
| Pole count and layout | Pole pairs, surface or interior, skew type | Determines how many planes must be measured |
| Defect of concern | What you are trying to catch, and its approximate size | Selects the method — this is the single most important input |
| Required resolution | Spatial resolution needed to resolve that defect | Directly incompatible with some array geometries |
| Throughput | Rotors per shift, or audit frequency | Decides array versus scanning |
| Pass/fail limits | The metric, its definition, and the limit | Prevents a report that cannot be judged |
| Report format | Required fields from §5.1, plus raw data | Makes the result usable in an audit |
| Data retention | Years, and the retrieval path | Determines whether the record survives the programme |
| Magnetized or unmagnetized | State of the rotor at measurement | Changes fixturing, safety and measurement approach entirely |
| On-site or laboratory | Whether the rotor can travel | Affects lead time and whether the array must be portable |
The second row is where most service enquiries go wrong. A customer asking for “a flux map” without naming the defect usually receives the method the supplier finds most convenient, which may be the wrong one. Naming the defect — a weak pole, a chipped corner, a skew error — determines the method before any commercial discussion begins.
Frequently asked questions
What is rotor surface magnetic field mapping? A measurement of the magnetic field distribution over a rotor’s surface, recorded as a map of normal and tangential components rather than a single value. The map is then reduced to metrics — per-pole flux spread, harmonic distortion, skew phase — that predict back-EMF variation, torque ripple, vibration and circulating currents.
Can I use a gauss meter for rotor inspection? For a coarse check on a single magnet, yes. For a rotor, no: a gauss meter reads one component at one point and cannot produce the distribution metrics that predict motor behaviour. It answers “is there field here” rather than “is this rotor going to whine”.
What is pole flux asymmetry and why does it matter? It is the spread in flux between poles, expressed relative to the rotor mean. Asymmetry produces unbalanced magnetic pull, which appears as pole-pass vibration and bearing load, and it drives circulating currents in windings with parallel paths. The definition — peak-to-peak over mean, or standard deviation — must be stated, because the two differ by a factor of two or more.
Is a Hall sensor array as accurate as a single-probe scanner? For detecting large-scale features such as a weak pole, yes. For small defects and high harmonics, no — resolution is fixed by channel pitch, and channels must be matched against each other. Arrays are the right tool for 100 % screening; scanning remains the reference method for qualification and dispute resolution.
Where does measurement uncertainty actually come from? Mostly from sensor positioning, not from sensor linearity. The field decays exponentially with distance from the surface, and high spatial harmonics decay far faster than the fundamental, so a small standoff error changes the harmonics by tens of percent. Any report should state the sensor-to-surface distance and how it was established.
What is a rotor flux sweep test? A scan that traverses the rotor surface in a continuous sweep rather than at discrete points, producing a high-resolution field profile along the path. It is the practical way to catch defects smaller than an array’s channel pitch, and it is normally used as an audit or failure-analysis method rather than for 100 % inspection.
How often should a production line be audit-scanned if it screens 100 % by array? There is no universal frequency. It should follow from the defects the array cannot resolve and their consequence: a defect that can cause a field failure justifies more frequent scanning than its historical occurrence rate implies. First article and any process change should always trigger a full reference map.
Can a flux map tell whether a rotor was damaged in service? Only against a baseline. A single map shows the current state; the comparison against a known-good map of the same design shows what has been lost. This is why reference maps captured at first article are worth keeping for the life of the programme.

FLUX MEASUREMENT SERVICE
Has a rotor failed a flux check and you need the cause, not the number?
Send the rotor, the drawing and the failed measurement. We will tell you which method can actually see your defect — single-probe scanning, a Hall array sweep or a full surface map — and what the resulting report has to contain to hold up in a supplier discussion.
- Reviewed by electromagnetic engineers, not a sales desk
- Typical reply within one business day
- A drawing and the failed measurement are enough to start
Prefer to talk it through? WhatsApp +86 188 6892 9496
Published 18 November 2026 · Reviewed by the JHHS MAG magnetizing engineering team
JHHS MAG (Ningbo Jiuheng Huisheng Technology Co., Ltd.) designs capacitor-discharge impulse magnetizers, magnetizing coils and fixtures, and automated magnetizing and testing systems for motor and magnetic component production. This article is part of the magnetizing knowledge base.
Continue reading
- Axial-flux rotor magnet assembly — gap-stack tolerance, 2–4 mm sector magnets and why a carbon-fibre wrap cannot hold a disc axially.
- Rotor magnetizing and testing systems — the station that charges and verifies the rotor in one cycle
- Halbach array rotor design — why the air-gap waveform matters more than the peak value
- Post-assembly magnetization for EV traction motor rotors — where the flux signature is created in the first place