Application Case 02 · Magnetizing service

Re-magnetizing Sm₂Co₁₇ Magnets Inside a PEEK-Overmolded Impeller

Scope: post-molding re-magnetization · fixture design · polarity verification

A manufacturer of encapsulated magnetic components for fluid-handling equipment builds an impeller of roughly 25 mm diameter, in which two Sm₂Co₁₇ magnets sit opposite each other in polarity, overmolded in PEEK, carried by an aluminium bracket and a tungsten-carbide shaft with a cobalt binder. The magnets are placed in the mold and the PEEK is injected around them. After molding, the measured field is clearly weaker than expected.

The question is not “why did it drop”. The question is whether it can be recovered — without opening the part, without disturbing the encapsulation, and without knowing what the correct field actually is yet.

Why injection molding costs you magnetization

Sm₂Co₁₇ is chosen exactly for this application because of its high-temperature capability: it can serve continuously well above 250 °C. But “high temperature capability” and “no loss during processing” are different statements.

PEEK is processed at melt temperatures well above 300 °C. A magnet encapsulated in the melt is exposed briefly to a temperature that sits above the material’s practical working limit, even if it stays far below its Curie point. What changes is not the crystal structure but the domain state: part of the alignment relaxes, and the operating point on the demagnetization curve drops. That loss is partly recoverable by re-magnetizing; a metallurgical change would not be.

This is the first thing to establish with a trial: is the loss reversible? If a re-magnetized sample comes back to its pre-molding level, the drop was thermal relaxation and the process can be fixed at the magnetizing station. If it does not, the process has to move upstream — and that changes the whole production strategy.

The real engineering problem: getting field into the part

Re-magnetizing an encapsulated assembly is not the same as magnetizing a bare magnet. Four things get in the way:

  • The aluminium bracket is conductive, not magnetic. It does not shield the magnet, but it does resist a fast field. A capacitor-discharge pulse lasting a few milliseconds is largely screened by eddy currents in the surrounding metal, so a short pulse can leave the magnet only partially charged. Longer pulse duration, or a different discharge profile, is often what actually fixes the part.
  • The tungsten-carbide shaft has a cobalt binder, and cobalt is ferromagnetic. The shaft is magnetically “soft” — it distorts the field locally, it can carry part of the flux away from the magnet, and it heats up in a pulsed field. Its position relative to the pole matters more than most people expect.
  • Two magnets with opposed polarity in one part. A single coil cannot magnetize them in opposite directions. The fixture needs either two independently driven coils, or a pole geometry that reverses the flux in one zone — a split-pole iron circuit with a defined gap between the two working areas.
  • The PEEK wall sets a stand-off. The working gap between pole face and magnet is fixed by the encapsulation thickness, so the fixture must be designed around that distance rather than the magnet’s own dimensions.

Why a Helmholtz coil cannot verify this part

This is the detail that most often gets missed in quotations for opposed-magnet assemblies.

A Helmholtz coil measures the net magnetic moment of whatever is inside it. If the two magnets point in opposite directions, their moments subtract. A perfectly good part and a part with one magnet almost dead can produce very similar net readings — and the coil cannot tell you which magnet is weak.

For this geometry the verification has to be per pole, per magnet position: a Hall probe at fixed measuring points, with the probe direction, the distance from the surface and the acceptance criterion all defined before the trial starts. Surface flux density at a defined point is the practical acceptance value; the net moment is useful as a secondary record, not as the deciding one.

Rule of thumb: if the assembly contains more than one magnet, define the acceptance method before defining the machine. Otherwise you can build a perfect magnetizer that produces parts nobody can inspect.

What a proper trial looks like

A sample trial on finished parts should answer five questions, in this order:

  1. Baseline. Measure the parts as received, per position, before touching them — so the loss is documented rather than assumed.
  2. Recovery limit. Re-magnetize at increasing field levels and record where saturation is reached. The curve, not a single number, tells you whether the fixture is adequate.
  3. Thermal effect. Log the temperature rise inside the part during charging. PEEK has a low thermal conductivity, and repeated pulses at production rate accumulate heat that a single lab shot does not reveal.
  4. Stability. Re-measure after 24–48 hours, and preferably after a thermal cycle toward the service temperature, to see whether the recovered state holds.
  5. Repeatability. Twenty parts, not two. The interesting number is the spread, not the best sample.

The process conclusion usually points one way

If the trial shows the loss is recoverable, the manufacturing route becomes: mold with magnets in a defined orientation, cool, then magnetize the finished part in a dedicated fixture. That route has three advantages over trying to magnetize through the mold:

  • No magnetizing hardware inside a hot mold, and no field acting on the melt;
  • The magnetizing step becomes a measurable, documented station — every part gets a record;
  • Parts that fail can be reworked once before being scrapped, if the encapsulation allows it.

What has to be settled first is the orientation guarantee: if the magnets are inserted by hand into the mold, the polarity convention must be fixed in writing, or the fixture will faithfully magnetize the wrong magnet in the wrong direction.

Frequently asked, in this type of project

Can a finished, encapsulated part be re-magnetized? Yes, in most cases — the field must penetrate the wall and any conductive bracket, which is a matter of pulse duration and fixture geometry rather than of magnet type.
Does the aluminium bracket shield the magnet? Aluminium is non-magnetic and does not shield static fields, but it does oppose fast pulses through eddy currents. Longer pulses penetrate better.
Do two opposed magnets need a special fixture? Yes. Either two independently driven coils or a split-pole circuit that reverses flux in one zone.
Can a fluxmeter check the result? Not reliably for an opposed pair — the moments subtract. Use a Hall probe at defined points for each magnet position.
Is post-molding magnetizing stable at 175 °C service? Sm₂Co₁₇ is capable, but the recovered state must be verified with a thermal cycle — that is part of the trial, not an assumption.
This application case describes an engineering evaluation carried out on customer-supplied parts. No customer identifiers, part numbers or drawing data are disclosed. Performance figures are design values and trial results, not guaranteed production data.
Re-magnetizing finished assemblies
We accept customer parts for sample trials and production re-magnetization, design the fixture around the encapsulation, and return a before/after inspection record for each magnet position.
Send us your part, your drawing and your acceptance question: sales001@jhhsmag.com

Scroll to Top
RFQ